12 kW fiber laser cutting chart for aluminium

Updated:

Short answer

At 12 kW the chart cuts aluminium from 1 to 40 mm: with nitrogen for 1–40 mm, with nitrogen or air for 35 mm. Speed runs from 45–50 m/min at 1 mm down to 0.15–0.2 m/min at 40 mm.

Cutting speed and gas pressure by thickness

ThicknessGasPressure, bar Speed, m/minPower, % Gas per 1 mFocus, mmHeight, mmNozzle
1 mm N₂1245–50100
2 mm N₂1230–35100
3 mm N₂1220–25100
4 mm N₂1218–20100
5 mm N₂1414–16100
6 mm N₂1410–12100
8 mm N₂146–8100
10 mm N₂144–6100
12 mm N₂162–3100
14 mm N₂161.5–2.5100
16 mm N₂161.3–2100
18 mm N₂161–1.6100
20 mm N₂160.8–1.2100
25 mm N₂160.5–0.7100
30 mm N₂180.25–0.3100
35 mm N₂ / air160.25100
40 mm N₂180.15–0.2100

Aluminium cutting at different power: what each kilowatt gives

Thickness 3 kW, m/min6 kW, m/min12 kW, m/min
1 mm 25–3030–4545–50
2 mm 15–1820–2530–35
4 mm 5–68–1018–20
5 mm 2.5–35–614–16
8 mm 0.6–0.71.5–26–8
10 mm 0.41–1.24–6

Common aluminium cutting defects

Severe striation curl (Bottom waviness)
Severe striation curl (Bottom waviness) Pronounced lag of drag lines in the lower portion of the cut (beam lag), resulting in a rough dross. Cause: Speed too high, power too low, focus too deep, assist gas pressure too low. First step: Decrease the speed (step 5%). Why is the cut edge rough and striated instead of smooth?
Porous dross along the sides
Porous dross along the sides Adhesion of loose, porous aluminum dross along the bottom edge. Cause: Focus set too deep, cutting speed set too high. First step: Raise the focus (step 0.5 mm). What settings does laser cutting aluminium need?
Incomplete cut on aluminum / Beam loss
Incomplete cut on aluminum / Beam loss The beam breaks down, forming an uncut groove with foamed aluminum melt. Cause: Feed rate too high, focus too low, assist gas pressure excessive. First step: Reduce the speed (step 5%). Fiber laser stopped cutting through the sheet — what is wrong?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Aluminium cutting charts at other power

Related questions

How thick aluminium can a 12 kW fiber laser cut?
The chart goes up to 40 mm, with nitrogen, at 0.15–0.2 m/min.
Which gas to cut aluminium with at 12 kW?
By the chart: with nitrogen for 1–40 mm, with nitrogen or air for 35 mm. The app picks the exact mode for your machine and nozzle.
Where are focus, nozzle and cutting height?
For every row of the chart they are in the SBM Laser Help app, together with alternative modes from other sources.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.