Short answer

A 3 kW fiber laser cuts 2 mm aluminium with nitrogen at 5–16 bar and 13.2–30 m/min. For this combination we have four regimes: the base one from the source maker’s table and three alternatives from other sources.

Aluminium cutting speed and gas pressure at 3 kW

Base regime · Aluminium · 2 mm · 3 kW
RFL-3000(50u), Cutting head focal length: Collimating 100/Focal 150
Gas
N₂
Gas pressure
12bar
Speed
15–18m/min
Power
100%
Frequency
1500–3500Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app
Alternative 1 · Aluminium · 2 mm · 3 kW
MAX, Head: BOCI BLT
Gas
Air
Gas pressure
5bar
Speed
30m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app
Alternative 2 · Aluminium · 2 mm · 3 kW
MAX 3000W, Head: OSPRI
Gas
N₂ / air
Gas pressure
16bar
Speed
13.2m/min
Power
100%
Frequency
5000Hz
Duty cycle
94%
Focus
in the app
Cutting height
in the app
Nozzle
in the app
Alternative 3 · Aluminium · 2 mm · 3 kW
MAX MFSC-3000X-50um, Head: none
Gas
N₂ / air
Gas pressure
16bar
Speed
17.5m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app

Which regime to start with

Cutting time and gas consumption per metre

At these speeds one metre of cut takes about 2–5 seconds. Nitrogen flow through the nozzle is about 13.6–38.6 m³ per hour, or 8–49 litres per metre of cut, not counting piercing.

Aluminium cutting speed chart: neighbouring thickness and power

Thickness · powerGasSpeed, m/min
1 mm · 3 kW N₂25–30
2 mm · 2 kW N₂ / air10
2 mm · 3 kW N₂15–18
2 mm · 4 kW N₂16–20
2 mm · 6 kW N₂20–25
3 mm · 3 kW N₂7–8
4 mm · 3 kW N₂5–6

Going from 3 kW to 4 kW gives about 9% more speed on 2 mm with nitrogen.

Common aluminium cutting defects with nitrogen

Incomplete cut on aluminum / Beam loss
Incomplete cut on aluminum / Beam loss The beam breaks down, forming an uncut groove with foamed aluminum melt. Cause: Feed rate too high, focus too low, assist gas pressure excessive. First step: Reduce the speed (step 5%). Fiber laser stopped cutting through the sheet — what is wrong?
Severe striation curl (Bottom waviness)
Severe striation curl (Bottom waviness) Pronounced lag of drag lines in the lower portion of the cut (beam lag), resulting in a rough dross. Cause: Speed too high, power too low, focus too deep, assist gas pressure too low. First step: Decrease the speed (step 5%). Why is the cut edge rough and striated instead of smooth?
Porous dross along the sides
Porous dross along the sides Adhesion of loose, porous aluminum dross along the bottom edge. Cause: Focus set too deep, cutting speed set too high. First step: Raise the focus (step 0.5 mm). What settings does laser cutting aluminium need?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Related questions

What is the thickest aluminium a 3 kW fiber laser cuts?
Our tables go up to 10 mm aluminium at 3 kW, at 0.4 m/min with nitrogen or air. The next thickness, 12 mm, starts from 4 kW.
Why is the speed a range?
Sheet surface, aluminium grade, gas purity and pressure at the nozzle and the state of the protective window all shift the result. Start at the lower value, make a test cut and raise the speed in 5% steps while the bottom edge stays clean.
Where are focus, cutting height and nozzle?
They depend on the cutting head and lens, so a single number is often wrong for your machine. The app shows the full regime and fits it to the machine you add to your profile.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.