Fiber laser settings for 3 mm brass at 3 kW

Updated:

Short answer

A 3 kW fiber laser cuts 3 mm brass with nitrogen at 14–16 bar and 5–6 m/min. For this combination we have two regimes: the base one from the source maker’s table and one alternative from another source.

Brass cutting speed and gas pressure at 3 kW

Base regime · Brass · 3 mm · 3 kW
RFL-3000(50u), Cutting head focal length: Collimating 100/Focal 150
Gas
N₂
Gas pressure
14bar
Speed
5–6m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app
Alternative · Brass · 3 mm · 3 kW
Raycus 3000W, Head: none
Gas
N₂ / air
Gas pressure
16bar
Speed
6m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app

Which regime to start with

Cutting time and gas consumption per metre

At these speeds one metre of cut takes about 10–12 seconds. Nitrogen flow through the nozzle is about 53.2–60.3 m³ per hour, or 148–177 litres per metre of cut, not counting piercing.

Brass cutting speed chart: neighbouring thickness and power

Thickness · powerGasSpeed, m/min
1 mm · 3 kW N₂20–28
2 mm · 3 kW N₂10–15
3 mm · 2 kW N₂ / air3
3 mm · 3 kW N₂5–6
3 mm · 4 kW N₂7–8
3 mm · 6 kW N₂12–14
4 mm · 3 kW N₂2.5–3
5 mm · 3 kW N₂1.8–2.2

Going from 3 kW to 4 kW gives about 36% more speed on 3 mm with nitrogen.

Common brass cutting defects with nitrogen

Beam reflection / Cut interruption on brass
Beam reflection / Cut interruption on brass The beam reflects off the mirror surface of brass, no through kerf is produced. Cause: High reflectivity of the alloy, feed rate too high. First step: Reduce the speed (step 5%). Fiber laser stopped cutting through the sheet — what is wrong?
Burn-through on the reverse side of brass
Burn-through on the reverse side of brass Metal tearouts and large droplets on the reverse side of the brass sheet. Cause: Assist gas pressure too low, power too high at feed rate too low. First step: Increase the assist gas pressure (step 1 bar). Where should the focus sit for stainless steel and mild steel?
Roughness on the bottom edge of brass
Roughness on the bottom edge of brass Pronounced striation and roughness in the lower portion of the brass part kerf. Cause: Focus position too high, gas pressure too high. First step: Raise the focus (step 0.5 mm). Why is the cut edge rough and striated instead of smooth?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Related questions

What is the thickest brass a 3 kW fiber laser cuts?
Our tables go up to 6 mm brass at 3 kW, at 0.8–1 m/min with nitrogen. The next thickness, 8 mm, starts from 4 kW.
Why is the speed a range?
Sheet surface, brass grade, gas purity and pressure at the nozzle and the state of the protective window all shift the result. Start at the lower value, make a test cut and raise the speed in 5% steps while the bottom edge stays clean.
Where are focus, cutting height and nozzle?
They depend on the cutting head and lens, so a single number is often wrong for your machine. The app shows the full regime and fits it to the machine you add to your profile.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.

Need the numbers for your exact machine?

See what is inside