12 kW fiber laser cutting chart for mild steel

Updated:

Short answer

At 12 kW the chart cuts mild steel from 1 to 40 mm: with nitrogen or air for 1–10 mm, with oxygen for 10–40 mm. Speed runs from 50–60 m/min at 1 mm down to 0.25–0.3 m/min at 40 mm.

Cutting speed and gas pressure by thickness

ThicknessGasPressure, bar Speed, m/minPower, % Gas per 1 mFocus, mmHeight, mmNozzle
1 mm N₂ / air1250–60100
2 mm N₂ / air1235–40100
3 mm N₂ / air1328–33100
4 mm N₂ / air1320–24100
5 mm N₂ / air1315–18100
6 mm N₂ / air1310–13100
8 mm N₂ / air137–10100
10 mm N₂ / air136–6.5100
O₂0.62–2.350
12 mm O₂0.61.8–263
14 mm O₂0.61.6–1.871
16 mm O₂0.61.5–1.679
18 mm O₂0.51.683
20 mm O₂0.61.3–1.4100
22 mm O₂0.70.9–1100
O₂0.71–1.2100
25 mm O₂0.70.7–0.9100
O₂0.70.8–1100
30 mm O₂1.30.4–0.5100
O₂0.80.7–0.8100
35 mm O₂0.70.45100
40 mm O₂1.50.25–0.3100

Mild steel cutting at different power: what each kilowatt gives

Thickness 3 kW, m/min6 kW, m/min12 kW, m/min
1 mm 28–3535–4550–60
4 mm 3–3.28–1020–24
8 mm 1.8–2.22.2–2.57–10
12 mm 0.9–11.9–2.11.8–2
18 mm 0.5–0.60.81.6
25 mm 0.540.50.8–1

Common mild steel cutting defects

Cut loss / Beam reflection
Cut loss / Beam reflection The beam breaks down, upward sparking occurs, and the metal is not cut through along the contour. Cause: Insufficient energy density, excessive cutting speed, incorrect focus. First step: Decrease the speed (step 5%). Fiber laser stopped cutting through the sheet — what is wrong?
Burn-throughs in the lower section (Breakthrough)
Burn-throughs in the lower section (Breakthrough) Burnout of metal at the bottom of the edge with formation of craters and buildup. Cause: Excessive cutting speed combined with insufficient assist gas pressure. First step: Decrease the cutting speed (step 5%). Where should the focus sit for stainless steel and mild steel?
Sharp hard dross
Sharp hard dross A sharp welded dross forms along the entire bottom edge. Cause: Focus set too deep, assist gas flow rate too low. First step: Lower/raise the focus (step 0.5 mm). How do I get rid of dross when cutting mild steel with oxygen?
Roughness with fine burrs
Roughness with fine burrs Rough cut surface across the full material thickness with formation of fine powdery dross on the bottom. Cause: Focus position set too high, oxygen pressure too low. First step: Raise/lower the focus (step 0.5 mm). Why is the cut edge rough and striated instead of smooth?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Mild steel cutting charts at other power

Related questions

How thick mild steel can a 12 kW fiber laser cut?
The chart goes up to 40 mm, with oxygen, at 0.25–0.3 m/min.
Which gas to cut mild steel with at 12 kW?
By the chart: with nitrogen or air for 1–10 mm, with oxygen for 10–40 mm. The app picks the exact mode for your machine and nozzle.
Where are focus, nozzle and cutting height?
For every row of the chart they are in the SBM Laser Help app, together with alternative modes from other sources.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.

Need the numbers for your exact machine?

See what is inside

SBM Laser Help carries cutting and piercing parameter tables by material, thickness and gas, photo diagnosis of cut defects, machine and chiller error codes, and gas consumption calculators. Free account, no card.