12 kW fiber laser cutting chart for stainless steel

Updated:

Short answer

At 12 kW the chart cuts stainless steel from 1 to 40 mm: with nitrogen for 1–40 mm, with air for 1–30 mm, with nitrogen or air for 22–35 mm. Speed runs from 50–60 m/min at 1 mm down to 0.15–0.2 m/min at 40 mm.

Cutting speed and gas pressure by thickness

ThicknessGasPressure, bar Speed, m/minPower, % Gas per 1 mFocus, mmHeight, mmNozzle
1 mm N₂1050–60100
Air1050–60100
2 mm N₂1240–45100
Air1040–45100
3 mm N₂1330–35100
Air1030–35100
4 mm N₂1222–26100
Air1022–28100
5 mm N₂1515–18100
Air1016–19100
6 mm N₂813–15100
Air1014–17100
8 mm N₂78–10100
Air109–11100
10 mm N₂56.5–7.5100
Air107–8100
12 mm N₂65–5.5100
Air105.5–6100
14 mm N₂63–3.5100
Air103.5–4100
16 mm N₂62–2.3100
Air102.2–2.4100
18 mm N₂61.3–1.5100
Air101.3–1.6100
20 mm N₂61.2–1.4100
Air101.2–1.5100
22 mm N₂ / air161.3100
25 mm N₂60.7–0.9100
Air100.7–1100
30 mm N₂100.25–0.3100
Air100.3–0.6100
35 mm N₂ / air160.25100
40 mm N₂150.15–0.2100

Stainless steel cutting at different power: what each kilowatt gives

Thickness 3 kW, m/min6 kW, m/min12 kW, m/min
1 mm 28–3540–5050–60
3 mm 7–1015–1830–35
4 mm 5–6.510–1222–28
6 mm 2–2.76–714–17
8 mm 1–1.23.5–3.89–11
16 mm 0.30.5–0.62.2–2.4

Common stainless steel cutting defects

Needle-like (fine) dross
Needle-like (fine) dross Fine needle-like burr along the full length of the bottom edge, easily removed. Cause: Cutting speed too high, focus set too deep. First step: Raise the focus (step 0.5 mm). Why does a fiber laser leave burr on stainless steel?
Long thick dross
Long thick dross Heavy, massive drops and 'icicles' of solidified metal on the bottom edge. Cause: Insufficient nitrogen/air pressure, excessive speed, buried focus. First step: Raise the focus (step 0.5 mm). Why does a fiber laser leave burr on stainless steel?
Plasma formation (Plasma cloud)
Plasma formation (Plasma cloud) Bright blue/violet glow above the cutting zone, reduction in beam penetration, melting of the top edge. Cause: Insufficient nitrogen pressure, cutting speed too high or power set too high. First step: Increase the nitrogen assist gas pressure (step 1 bar). Where should the focus sit for stainless steel and mild steel?
Bottom edge melting and darkening
Bottom edge melting and darkening The bottom portion of the edge has a dark blue/brown color (oxidation) with visible signs of overheating. Cause: Low nitrogen pressure, insufficient gas flow to cool the kerf zone. First step: Increase the nitrogen assist gas pressure (step 1 bar). Why does a fiber laser leave burr on stainless steel?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Stainless steel cutting charts at other power

Related questions

How thick stainless steel can a 12 kW fiber laser cut?
The chart goes up to 40 mm, with nitrogen, at 0.15–0.2 m/min.
Which gas to cut stainless steel with at 12 kW?
By the chart: with nitrogen for 1–40 mm, with air for 1–30 mm, with nitrogen or air for 22–35 mm. The app picks the exact mode for your machine and nozzle.
Where are focus, nozzle and cutting height?
For every row of the chart they are in the SBM Laser Help app, together with alternative modes from other sources.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.

Need the numbers for your exact machine?

See what is inside

SBM Laser Help carries cutting and piercing parameter tables by material, thickness and gas, photo diagnosis of cut defects, machine and chiller error codes, and gas consumption calculators. Free account, no card.