Stainless is cut with high-pressure nitrogen for a clean, oxide-free edge, and most stainless problems trace back to gas pressure, gas purity or focus. The answers below explain why burr forms on the bottom edge and when oxygen cutting of stainless is acceptable. Cutting parameters by power and thickness are listed below; focus, cutting height and nozzle for each are in SBM Laser Help.
All cutting modes by metal, thickness, gas and laser power, with alternative modes, are in the SBM Laser Help parameter tables.Parameter tables in the app →
Burr on stainless cut with nitrogen almost always means the melt is not being blown out fast enough: cutting speed too low for the power, nitrogen pressure or purity too low, a worn or off-centre nozzle, or focus sitting too high in the sheet. Start with nozzle condition and gas pressure — they explain most burr cases in a shop.
Read the answer →Yes, and it is faster and cheaper than nitrogen, but the edge oxidises: it turns dark or straw-coloured and loses corrosion resistance right at the cut. It suits thick plate, structural parts and anything that gets ground or painted afterward — not visible or weld-critical parts.
Read the answer →



When a machine that used to cut through stops penetrating, the beam is losing energy on its way to the sheet or landing in the wrong place. In order of likelihood: dirty or cracked protective glass, worn nozzle, focus drift, gas pressure loss, and only then the source itself.
Read the answer →Striations are the fingerprint of an unstable melt front. Coarse, dragging lines mean the melt cannot keep up — usually speed, focus or gas dynamics. Fine even lines are normal and cannot be removed entirely; what you control is their depth and how far down the edge they start.
Read the answer →Spatter is melt ejected back up toward the head instead of down through the kerf — usually from piercing thick material too aggressively, standoff set too low, or pressure too high for the nozzle. It clogs the nozzle fast, and a clogged nozzle then makes spatter worse.
Read the answer →Taper means the beam is not delivering a straight-walled cut through the full thickness: usually focus sitting at or above the surface on thick material, speed slightly too high, or a worn lens spreading the beam. It shows up mostly on plate over 8–10 mm, where the beam has more depth to travel through.
Read the answer →SBM Laser Help carries cutting and piercing parameter tables by material, thickness and gas, photo diagnosis of cut defects, machine and chiller error codes, and gas consumption calculators. Free account, no card.