Answers for the operator who is dialling in a new material or thickness: where to put the focus for oxygen and nitrogen cutting, how long to pierce, how cutting speed falls as the sheet gets thicker, which nozzle diameter to choose, what kerf width means for part accuracy and how to check beam alignment. Numbers are ranges for a typical 3–6 kW fiber source. Exact tables by machine, material and thickness are in SBM Laser Help.
All cutting modes by metal, thickness, gas and laser power, with alternative modes, are in the SBM Laser Help parameter tables.Parameter tables in the app →
The rule of thumb: cutting with nitrogen, the focus goes below the surface — roughly a third to two thirds of the thickness down. Cutting mild steel with oxygen, the focus sits at the surface or slightly above it. Thin sheet under 2 mm is close to zero in both cases.
Read the answer →Piercing time grows with thickness: on a 6 kW fiber, thin sheet pierces in well under a second, 10 mm in roughly one second, and 20 mm plate needs one to three seconds with ramped power. Thick material pierces on oxygen at low pressure with the focus higher than the cutting focus, then switches to the cutting parameter set.
Read the answer →Speed falls sharply with thickness and depends on the gas: a 6 kW fiber cuts 1 mm stainless with nitrogen at 30–40 m/min, 6 mm at around 5 m/min, and 10 mm at 2–3 m/min. Mild steel with oxygen is slower on thin sheet but keeps cutting into 20 mm plate where nitrogen becomes impractical.
Read the answer →Nozzle diameter follows thickness and gas: small single nozzles of 1.0–1.5 mm for oxygen cutting of mild steel, larger double nozzles of 1.4–3.0 mm for nitrogen cutting where a wide, high-pressure jet must clear the melt. Too large a nozzle wastes gas and softens the jet; too small starves the kerf.
Read the answer →Kerf is the width of material the beam actually removes — narrower than a saw cut but not zero. On a 3–6 kW fiber it typically runs 0.1–0.3 mm on thin sheet and grows to 0.4–0.6 mm past 10 mm, driven mostly by nozzle diameter, focus and cutting gas.
Read the answer →Taper means the beam is not delivering a straight-walled cut through the full thickness: usually focus sitting at or above the surface on thick material, speed slightly too high, or a worn lens spreading the beam. It shows up mostly on plate over 8–10 mm, where the beam has more depth to travel through.
Read the answer →Aluminium cuts with nitrogen at high pressure, similar to stainless, but its high reflectivity and thermal conductivity mean it needs more power margin for the same thickness and is far less forgiving of a dirty lens or slightly off focus — both cause a lost cut, not just a quality drop.
Read the answer →Misalignment shows up as quality that differs by direction or position on the table, not as a single obvious fault: cuts fine on one axis but rough on the other, or good near the centre and worse toward the edges. A burn-paper test at two points on the beam path finds it faster than guessing from the cut alone.
Read the answer →SBM Laser Help carries cutting and piercing parameter tables by material, thickness and gas, photo diagnosis of cut defects, machine and chiller error codes, and gas consumption calculators. Free account, no card.