Fiber laser settings for 2 mm stainless steel at 1 kW

Updated:

Short answer

A 1 kW fiber laser cuts 2 mm stainless steel with nitrogen or air at 14–16 bar and 6–7 m/min. For this combination we have two regimes: the base one from the source maker’s table and one alternative from another source.

Stainless steel cutting speed and gas pressure at 1 kW

Base regime · Stainless steel · 2 mm · 1 kW
1000W(50u), Cutting head focal length: Collimating 100/Focal 125
Gas
N₂ / air
Gas pressure
14bar
Speed
6.5–7m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app
Alternative · Stainless steel · 2 mm · 1 kW
Raycus 1000W, Head: none
Gas
N₂ / air
Gas pressure
16bar
Speed
6m/min
Power
100%
Frequency
5000Hz
Duty cycle
100%
Focus
in the app
Cutting height
in the app
Nozzle
in the app

Which regime to start with

Cutting time and gas consumption per metre

At these speeds one metre of cut takes about 9–10 seconds. Nitrogen or air flow through the nozzle is about 34–38.6 m³ per hour, or 81–107 litres per metre of cut, not counting piercing.

Stainless steel cutting speed chart: neighbouring thickness and power

Thickness · powerGasSpeed, m/min
0.8 mm · 1 kW N₂ / air20
1 mm · 1 kW N₂ / air21–23
2 mm · 500 W N₂ / air2.6–2.8
2 mm · 1 kW N₂ / air6.5–7
2 mm · 1.5 kW N₂ / air7
2 mm · 2 kW N₂ / air10
3 mm · 1 kW N₂ / air2.3–2.5
4 mm · 1 kW N₂ / air1.4–1.6

Common stainless steel cutting defects with nitrogen or air

Needle-like (fine) dross
Needle-like (fine) dross Fine needle-like burr along the full length of the bottom edge, easily removed. Cause: Cutting speed too high, focus set too deep. First step: Raise the focus (step 0.5 mm). Why does a fiber laser leave burr on stainless steel?
Long thick dross
Long thick dross Heavy, massive drops and 'icicles' of solidified metal on the bottom edge. Cause: Insufficient nitrogen/air pressure, excessive speed, buried focus. First step: Raise the focus (step 0.5 mm). Why does a fiber laser leave burr on stainless steel?
Plasma formation (Plasma cloud)
Plasma formation (Plasma cloud) Bright blue/violet glow above the cutting zone, reduction in beam penetration, melting of the top edge. Cause: Insufficient nitrogen pressure, cutting speed too high or power set too high. First step: Increase the nitrogen assist gas pressure (step 1 bar). Where should the focus sit for stainless steel and mild steel?
Bottom edge melting and darkening
Bottom edge melting and darkening The bottom portion of the edge has a dark blue/brown color (oxidation) with visible signs of overheating. Cause: Low nitrogen pressure, insufficient gas flow to cool the kerf zone. First step: Increase the nitrogen assist gas pressure (step 1 bar). Why does a fiber laser leave burr on stainless steel?

Not sure which one you have? Send a photo of the edge to the app and it names the defect and the fix.

Related questions

What is the thickest stainless steel a 1 kW fiber laser cuts?
Our tables go up to 6 mm stainless steel at 1 kW, at 0.5–0.6 m/min with nitrogen or air. The next thickness, 8 mm, starts from 2 kW.
Why is the speed a range?
Sheet surface, stainless steel grade, gas purity and pressure at the nozzle and the state of the protective window all shift the result. Start at the lower value, make a test cut and raise the speed in 5% steps while the bottom edge stays clean.
Where are focus, cutting height and nozzle?
They depend on the cutting head and lens, so a single number is often wrong for your machine. The app shows the full regime and fits it to the machine you add to your profile.

Ranges are given for a typical 3–6 kW fiber machine with a clean beam path. Always verify against your machine manufacturer’s table before production.